Product details | ||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Composition (content in mass %) |
Au 59.3 Ag 22.9 Pt 0.6 Pd 3.7 Cu 13.0 Zn 0.4 Ir x Ru x |
|||||||||||||
Type | 4(v), 3(w) | |||||||||||||
Shade | Yellow | |||||||||||||
Indication |
Inlays, cervical restorations MOD Inlays Crowns Bridges Milling technique Partial dentures Cast posts Implant restorations |
|||||||||||||
Article Code | 13900000 |
Technical data melting and casting | ||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Melting range (1) |
Solidus 870°C Liquidus 920°C |
|||||||||||||
Preheating temperature | 700°C | |||||||||||||
Casting temperature | 1050°C | |||||||||||||
Crucible |
Graphite |
|||||||||||||
Density (1) | 14.1 g/cm3 | |||||||||||||
Hardness, HV5 | 160 (w/k), 265 (v), 265 (s) | |||||||||||||
0.2 % proof stress(1), MPa(2) | 340 (w/k), 780 (v) | |||||||||||||
Elongation(1) % | 38 (w/k), 6 (v) | |||||||||||||
Elastic modulus(1), GPa(2) | 103 |
Ceramic firing | ||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
CTE | --- | |||||||||||||
Oxide firing | --- | |||||||||||||
Soft annealing | 750°C / 15 min. | |||||||||||||
Processing after oxide firing | --- | |||||||||||||
Cooling after ceramic firing (Relexation cooling is recommended for lang span, bulky frameworks) | --- | |||||||||||||
Hardening | 400°C / 15 min. |
Prior to Ceramic Firing | ||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Solder |
Hera Lot 800 + Maingold / Hera Lot 750 |
|||||||||||||
Solder colour: yellow | ||||||||||||||
After Ceramic Firing | ||||||||||||||
Solder | Hera Lot 800 + Maingold / Hera Lot 750 | |||||||||||||
Flux** | Solder colour: yellow | |||||||||||||
Alloy also available as Laser weiding wire | ||||||||||||||
Ø 0.5 mm x 200 mm | + | |||||||||||||
Ø 0.3 mm x 200 mm | + |